ZDROJOVÝ PODKLAD
Uložený text
https://drive.google.com/file/d/1wFKJmBAlD2ng6aUQdBrmS3QB1rKB4f8W/view ↗ A L U M I N U M E X T R U S I O N P R O C E DU R E # 01
Revision 01
ALUMINUM EXTRUSION Page 1/4
A. OBJECTIVE(S)
This specification has the objective to define the most common aluminium extrusion defects, aesthetic
acceptance criteria as well as the standards that different products must meet from a chemical
composition and mechanical performance standpoint. Any aluminium extruded component part of Taiga
vehicles falls within the scope of this specification. Instructions regarding the procedure to follow when
inspecting components are presented in this document.
B. AESTHETICAL AND STRUCTURAL DEFECTS
In order to ensure that Taiga requirements are met, parts shall be inspected at the supplier. Parts
delivered to Taiga shall be free from any of the following surface and structural defects:
Blisters
Pick-up defects
Die lines and scratches
Burn marks
Pipe formation
Internal or surface cracking
Burr and sharp edges
Note that all these defects are defined and illustrated in Annex A.
Furthermore, any aluminium extrusion part that is to be coated must meet the aesthetical acceptance
criteria defined in Table 1 of Taiga’s Coating and Plastics Aesthetic Specification. This document can be
supplied upon request.
C. APPLICABLE STANDARDS/SPECIFICATIONS
The mechanical and chemical composition requirements communicated in section D of this document
are based on the standards/specifications defined in Table 1 below. The applicable standard must be
selected based on the type of product that is to be inspected.
Product Specification
Wire, rod, bar, profiles and tube; extruded ASTM B221
Tube; extruded, seamless ASTM B241
TABLE 1: Applicable specification based on product type
D. MECHANICAL PROPERTIES AND CHEMICAL COMPOSTION REQUIREMENTS
D.1 Sampling
An inspection lot shall consist of an identifiable quantity of material of the same mill form, alloy, temper,
and nominal dimensions traceable to a heat-treat lot or lots (only applicable for heat treated material)
and subjected to inspection at one time.
A L U M I N U M E X T R U S I O N P R O C E DU R E # 01
Revision 01
ALUMINUM EXTRUSION Page 2/4
For each delivery, chemical composition and mechanical properties compliance must be demonstrated
as defined below.
D.2 Chemical Composition
Samples for chemical analysis shall be taken from the material by drilling, sawing, milling, turning, or
clipping a representative piece or pieces to obtain a prepared sample of not less than 75 g. Sampling
shall be in accordance with Practice ASTM E 55. Samples can also be obtained when ingots are poured.
The material composition shall meet the chemical composition limits defined in the Table of the relevant
ASTM Standard (see section C for more details). The chemical composition analysis must be performed
using a relevant chemical or spectrochemical method. Other methods may be used upon Taiga’s
approval.
D.3 Mechanical Properties
Samples for mechanical properties shall have the relevant testing Geometry of test specimens and the
location in the product from which they are taken shall be as specified in Test Methods B 557.
A tension test is to be performed based on the ASTM B557 Method. The material tensile properties
(tensile strength, yield strength and elongation) shall be conformed to the limits defined in the Table of
the relevant ASTM Standard (see section C for more details).
A L U M I N U M E X T R U S I O N P R O C E DU R E # 01
Revision 01
ALUMINUM EXTRUSION Page 3/4
ANNEX A: DEFINITION OF AESTHETICAL AND STRUCTURAL DEFECTS
Blisters: Bubbles and irregular shapes formed on extruded aluminum. This is caused by the aluminum
that gets sticked to the fixed dummy fitted in the stem of extrusion press.
Pick-up defect: Intermittent score lines of varying lengths between 3 mm and 12 mm and often
terminates in a fleck of aluminum debris referred to as pick-up deposit. The problem is usually thought
to be enhanced by inclusions in the cast billet or inadequate homogenization treatment.
Die lines and scratches: Longitudinal depressions or protrusions formed on the surface of the extruded
material due to imperfections on the die surface. These imperfections could include inclusions, irregular
marks or contaminations.
Burn marks: Black burn marks formed on the section surface during extrusion due to the creation of high
local temperature induced by the presence of inclusions or oils in the billet material.
A L U M I N U M E X T R U S I O N P R O C E DU R E # 01
Revision 01
ALUMINUM EXTRUSION Page 4/4
Pipe formation: Also called extrusion defect, fishtailing, or back-end defect. Annular separation in the
cross section (due to division into an inner core and an external zone) in the rear of the extrusion.
Internal or surface cracking: Cracks are attributed to a state of tensile stress at the centerline of the
deformation zone in the die or at areas of melting.
F. REVISION HISTORY
Revision Signed by
Changes / Notes / Comments
Date
Rev 01, header , burrs and edges removal David Maltais
2022-06-21
and section F were added.
[READING ORDER TEXT]
ALUMINUM EXTRUSION PROCEDURE # 01
ALUMINUM EXTRUSION
Revision 01
Page 1 / 4
A. OBJECTIVE(S)
This specification has the objective to define the most common aluminium extrusion defects, aesthetic
acceptance criteria as well as the standards that different products must meet from a chemical
composition and mechanical performance standpoint. Any aluminium extruded component part of Taiga
vehicles falls within the scope of this specification. Instructions regarding the procedure to follow when
inspecting components are presented in this document.
B. AESTHETICAL AND STRUCTURAL DEFECTS
In order to ensure that Taiga requirements are met, parts shall be inspected at the supplier. Parts
delivered to Taiga shall be free from any of the following surface and structural defects:
Blisters
Pick-up defects
Die lines and scratches
Burn marks
Pipe formation
Internal or surface cracking
Burr and sharp edges
Note that all these defects are defined and illustrated in Annex A.
Furthermore, any aluminium extrusion part that is to be coated must meet the aesthetical acceptance
criteria defined in Table 1 of Taiga’s Coating and Plastics Aesthetic Specification. This document can be
supplied upon request.
C. APPLICABLE STANDARDS/SPECIFICATIONS
The mechanical and chemical composition requirements communicated in section D of this document
are based on the standards/specifications defined in Table 1 below. The applicable standard must be
selected based on the type of product that is to be inspected.
Product Specification
Wire, rod, bar, profiles and tube; extruded ASTM B221
Tube; extruded, seamless ASTM B241
TABLE 1: Applicable specification based on product type
D. MECHANICAL PROPERTIES AND CHEMICAL COMPOSTION REQUIREMENTS
D.1 Sampling
An inspection lot shall consist of an identifiable quantity of material of the same mill form, alloy, temper,
and nominal dimensions traceable to a heat-treat lot or lots (only applicable for heat treated material)
and subjected to inspection at one time.ALUMINUM EXTRUSION PROCEDURE # 01
ALUMINUM EXTRUSION
Revision 01
Page 2 / 4
For each delivery, chemical composition and mechanical properties compliance must be demonstrated
as defined below.
D.2 Chemical Composition
Samples for chemical analysis shall be taken from the material by drilling, sawing, milling, turning, or
clipping a representative piece or pieces to obtain a prepared sample of not less than 75 g. Sampling
shall be in accordance with Practice ASTM E 55. Samples can also be obtained when ingots are poured.
The material composition shall meet the chemical composition limits defined in the Table of the relevant
ASTM Standard (see section C for more details). The chemical composition analysis must be performed
using a relevant chemical or spectrochemical method. Other methods may be used upon Taiga’s
approval.
D.3 Mechanical Properties
Samples for mechanical properties shall have the relevant testing Geometry of test specimens and the
location in the product from which they are taken shall be as specified in Test Methods B 557.
A tension test is to be performed based on the ASTM B557 Method. The material tensile properties
(tensile strength, yield strength and elongation) shall be conformed to the limits defined in the Table of
the relevant ASTM Standard (see section C for more details).ALUMINUM EXTRUSION PROCEDURE # 01
ALUMINUM EXTRUSION
Revision 01
Page 3 / 4
ANNEX A: DEFINITION OF AESTHETICAL AND STRUCTURAL DEFECTS
Blisters: Bubbles and irregular shapes formed on extruded aluminum. This is caused by the aluminum
that gets sticked to the fixed dummy fitted in the stem of extrusion press.
Pick-up defect: Intermittent score lines of varying lengths between 3 mm and 12 mm and often
terminates in a fleck of aluminum debris referred to as pick-up deposit. The problem is usually thought
to be enhanced by inclusions in the cast billet or inadequate homogenization treatment.
Die lines and scratches: Longitudinal depressions or protrusions formed on the surface of the extruded
material due to imperfections on the die surface. These imperfections could include inclusions, irregular
marks or contaminations.
Burn marks: Black burn marks formed on the section surface during extrusion due to the creation of high
local temperature induced by the presence of inclusions or oils in the billet material.ALUMINUM EXTRUSION PROCEDURE # 01
ALUMINUM EXTRUSION
Revision 01
Page 4 / 4
Pipe formation: Also called extrusion defect, fishtailing, or back-end defect. Annular separation in the
cross section (due to division into an inner core and an external zone) in the rear of the extrusion.
Internal or surface cracking: Cracks are attributed to a state of tensile stress at the centerline of the
deformation zone in the die or at areas of melting.
F. REVISION HISTORY
Revision
Date
Changes / Notes / Comments
Signed by
2022-06-21
Rev 01, header , burrs and edges removal
and section F were added.
David MaltaisIdentifikace uložené verze