← Přehled firem
Získáno 24. 10. 2026 · 23:52
                                                  C O A T I N G A N D P L A ST I C S S P E C I F I C A T I O N #    01
                                                                                                                   JUN 21
                                                                                                   Revision
                                                      AESTHETIC                                                     2022
                                                                                                     Page           1/5




    A. SCOPE AND DESCRIPTION
This specification has the objective to define the aesthetic acceptance criteria of various painted
components (liquid or powder coating) and plastic parts of the Snowmobile and Watercraft products.
Instructions regarding the procedure to follow when inspecting components are also presented in this
document.

    B. PROCEDURE
All parts must be inspected with a viewing distance of 18-24 inches (45 – 60 cm), “waist high” or about
26-30 inches (66 – 76 cm) from the floor. Illumination should be cool white fluorescent having a minimum
light intensity of 100 Foot-candle. If no defect is observed, the part is deemed acceptable. If a defect is
observed under these conditions, the part must be examined in a more exhaustive way, using closer
examination to properly classify the defect as per Tables 1 and 2.

For each defect encountered on a part, the evaluator must refer to Tables 1, 2 and use the following
methodology:

    1. Use the transparent film template to compare the defect against the maximum size allowed,
       depending on the surface class.
    2. Use the transparent film template to compare spacing between defects against the minimum
       distance allowed, depending on the surface class.
    3. For orange peel, compare the part against the P.C.I sample which is related to the maximum
       orange peel level that can be allowed.
    4. Evaluate the colour difference and the gloss as per Tables 3 and 4.


The 3 surface classes are classified as follow:

“A” SURFACE –Areas most prominent to the observer or most likely to be noticed at first glance.

“B” SURFACE -- Areas not visible except by special effort by the observer under normal conditions.

“C” SURFACE – Areas normally not seen by observer or those not seen except by disassembly.
                                                  C O A T I N G A N D P L A ST I C S S P E C I F I C A T I O N #      01
                                                                                                                    JUN 21
                                                                                                    Revision
                                                      AESTHETIC                                                      2022
                                                                                                     Page            2/5


   C. ACCEPTANCE CRITERIA
COATING DEFECTS                                          MINIMUM DISTANCE REQUIRED BETWEEN DEFECTS
DEFECT                 MAXIMUM DIMENSION                         A                              B                          C
                       ACCEPTED
Encased impurities        1 mm diameter                     150 mm                         100 mm                     50 mm
                             2 mm diameter               Not allowed                       150 mm                    100 mm

Craters and voids            2 mm diameter               Not allowed                       150 mm                    100 mm

Fisheyes                     2 mm diameter               Not allowed                    Not allowed                  100 mm

Pinholes                  0.5 mm diameter                     2 mm                           1 mm                    Allowed

Fumes                              NA                    Not allowed                    Not allowed                  Allowed

Orange Peel                        NA                 P.C.I 7 minimum                P.C.I 6 minimum                Not allowed

Paint Coverage                     NA                    Full coverage                 Full coverage               80% coverage,
                                                                                                                    minimum*
Drips                        25 mm length                Not allowed                    Not allowed                  100 mm

                                         * Conversion coating/pre-treatment shall cover 100% of the part to prevent corrosion.

                 TABLE 1: Defects and acceptance criteria for coatings on metallic and plastic substrates



    DEFECT               A               B                   C                                      Notes

Blisters             Not allowed    Not allowed         Allowed         Blisters must not interfere with
                                                                        assembly or functionality.
Burn marks           Not allowed    Not allowed         Allowed         Burn marks allowed for C surfaces if
                                                                        delamination doesn’t propagate.
Gate marks           Not allowed    Not allowed         Allowed         Burn marks must not interfere with
                                                                        assembly or functionality.
Splay marks          Not allowed    Not allowed         Allowed         Material must be dried to prevent splay
                                                                        marks.
Jetting              Not allowed    Not allowed         Allowed

Sink Marks           Not allowed    Not allowed         Allowed         Must not affect structural integrity.

Weld lines           Not allowed    Not allowed         Allowed         Must not affect structural integrity.

              TABLE 2: Defects and acceptance criteria for plastic parts not to be painted
                                                  C O A T I N G A N D P L A ST I C S S P E C I F I C A T I O N #       01
                                                                                                                   JUN 21
                                                                                                   Revision
                                                      AESTHETIC                                                     2022
                                                                                                     Page           3/5


Scratches and discontinuities (Streaks, dents, etc.): Defects reaching the substrate, or the primer are not
allowed. Scratches and dent that can be felt by the back of the nail are not allowed. Scratches and dents
shall only be visible when viewed from a certain angle.

                                         MAXIMUM ∆E*ab VALUE
                                      MEASURED AS PER ASTM D2244
                                              A                  B                                                 C
 Colour difference when compared            ≤1                     ≤2                                      Values ≥ 2 are
 to reference sample                                                                                          allowed
                           Table 3: Maximum colour differences allowed



                   Finish                               Gloss Value (ASTM D523)

                   High gloss                           76 gloss units and up @60°

                   Semi gloss                           51-75 gloss units @20°

                   Matte                                30-50 gloss units @20°

                                           Table 4: Gloss values

    D. DEFECT DEFINITIONS
Encased impurities: Dirt or dust in the finish; may cause small dents to the surface of the finish.

Craters and voids: Spots where paint on the coated surface has receded, often concentrically, to leave a
spot with no paint. Cratering is caused by incompatible foreign materials either in the paint or substrate.

Fisheyes: Circular voids or separation in the coating. Fisheyes are small, crater-like openings in the finish
after it has been applied. They are usually caused by oil, grease, or silicon on the substrate.

Pinholes: A pinhole is a pore-like penetration that is present in paints and coatings due to the entrapment
of moisture, air, solvents, or other fluids.

Fumes: Contamination from paint fumes. This generally means that small points from another color can
appear on the finish.

Orange Peel: This defect is a rippling of the cured finishing material and appears rough and uneven, much
like the skin of an orange or the exterior of basketball.

Paint Coverage: Ability of a coating to cover the surface on which it’s applied.

Drips: Trace made by the paint while flowing on the substrate

Blisters: Small bubbles or voids on the surface of a molded part caused by trapped gases in the part that
could not escape before the surface began to “skin “during the molding process.
                                                   C O A T I N G A N D P L A ST I C S S P E C I F I C A T I O N #     01
                                                                                                                     JUN 21
                                                                                                    Revision
                                                       AESTHETIC                                                      2022
                                                                                                      Page            4/5


Burn marks: Black or rust discoloration on an edge or surface, caused by high temperature gases.

Gate marks: Indentation or depression that occurs in the same location of every part due the mold
injection point.

Splay marks: A “splash-like” appearance (or spray pattern) on the surface of a molded part. Often due to
moisture in raw material.

Jetting: Jetting refers to a situation where molten plastic fails to stick to the mold surface due to the speed
of injection.

Sink Marks: Areas in a molded part where the surface is deformed into a depression. The depressions
typically occur in areas of thick geometry and are caused by uneven cooling.

Weld lines: Areas of a molded part where the molten material has converged after splitting off into two
or more directions in a mold. The hair-like weld line is the result of weak material bonding, which lowers
the strength of the part.

    E. INSPECTION STENCIL




     0.5mm             0.75mm              1mm                 1.5mm                     2mm                        5mm




150 mm




100 mm




50 mm
                                           C O A T I N G A N D P L A ST I C S S P E C I F I C A T I O N #    01
                                                                                                            JUN 21
                                                                                            Revision
                                               AESTHETIC                                                     2022
                                                                                              Page           5/5




  F. REVISION HISTORY
Revision                                                        Signed by
             Changes / Notes / Comments
Date
2022-06-21     Rev 01, header and section F were added.         David Maltais


[READING ORDER TEXT]
COATING AND PLASTICS SPECIFICATION # 01
AESTHETIC
Revision
JUN 21
2022
Page 1 / 5
A. SCOPE AND DESCRIPTION
This specification has the objective to define the aesthetic acceptance criteria of various painted
components (liquid or powder coating) and plastic parts of the Snowmobile and Watercraft products.
Instructions regarding the procedure to follow when inspecting components are also presented in this
document.
B. PROCEDURE
All parts must be inspected with a viewing distance of 18-24 inches (45 – 60 cm), “waist high” or about
26-30 inches(66 – 76 cm)from the floor.Illumination should be coolwhite fluorescent having aminimum
light intensity of 100 Foot-candle. If no defect is observed, the part is deemed acceptable. If a defect is
observed under these conditions, the part must be examined in a more exhaustive way, using closer
examination to properly classify the defect as per Tables 1 and 2.
For each defect encountered on a part, the evaluator must refer to Tables 1, 2 and use the following
methodology:
1. Use the transparent film template to compare the defect against the maximum size allowed,
depending on the surface class.
2. Use the transparent film template to compare spacing between defects against the minimum
distance allowed, depending on the surface class.
3. For orange peel, compare the part against the P.C.I sample which is related to the maximum
orange peel level that can be allowed.
4. Evaluate the colour difference and the gloss as per Tables 3 and 4.
The 3 surface classes are classified as follow:
“A” SURFACE –Areas most prominent to the observer or most likely to be noticed at first glance.
“B” SURFACE -- Areas not visible except by special effort by the observer under normal conditions.
“C” SURFACE – Areas normally not seen by observer or those not seen except by disassembly.COATING AND PLASTICS SPECIFICATION # 01
AESTHETIC
Revision
JUN 21
2022
Page 2 / 5
C. ACCEPTANCE CRITERIA
COATING DEFECTS MINIMUM DISTANCE REQUIRED BETWEEN DEFECTS
DEFECT MAXIMUM DIMENSION
ACCEPTED
A B C
Encased impurities 1 mm diameter 150 mm 100 mm 50 mm
2 mm diameter Not allowed 150 mm 100 mm
Craters and voids 2 mm diameter Not allowed 150 mm 100 mm
Fisheyes 2 mm diameter Not allowed Not allowed 100 mm
Pinholes 0.5 mm diameter 2 mm 1 mm Allowed
Fumes NA Not allowed Not allowed Allowed
Orange Peel NA P.C.I 7 minimum P.C.I 6 minimum Not allowed
Paint Coverage NA Full coverage Full coverage 80% coverage,
minimum*
Drips 25 mm length Not allowed Not allowed 100 mm
* Conversion coating/pre-treatment shall cover 100% of the part to prevent corrosion.
TABLE 1: Defects and acceptance criteria for coatings on metallic and plastic substrates
TABLE 2: Defects and acceptance criteria for plastic parts not to be painted
DEFECT A B C Notes
Blisters Not allowed Not allowed Allowed Blisters must not interfere with
assembly or functionality.
Burn marks Not allowed Not allowed Allowed Burn marks allowed for C surfaces if
delamination doesn’t propagate.
Gate marks Not allowed Not allowed Allowed Burn marks must not interfere with
assembly or functionality.
Splay marks Not allowed Not allowed Allowed Material must be dried to prevent splay
marks.
Jetting Not allowed Not allowed Allowed
Sink Marks Not allowed Not allowed Allowed Must not affect structural integrity.
Weld lines Not allowed Not allowed Allowed Must not affect structural integrity.COATING AND PLASTICS SPECIFICATION # 01
AESTHETIC
Revision
JUN 21
2022
Page 3 / 5
Scratches and discontinuities (Streaks, dents, etc.): Defects reaching the substrate, or the primer are not
allowed. Scratches and dent that can be felt by the back of the nail are not allowed. Scratches and dents
shall only be visible when viewed from a certain angle.
MAXIMUM ∆E*
ab VALUE
MEASURED AS PER ASTM D2244
A B C
Colour difference when compared
to reference sample
≤ 1 ≤ 2 Values ≥ 2 are
allowed
Table 3: Maximum colour differences allowed
Finish Gloss Value (ASTM D523)
High gloss 76 gloss units and up @60°
Semi gloss 51-75 gloss units @20°
Matte 30-50 gloss units @20°
Table 4: Gloss values
D. DEFECT DEFINITIONS
Encased impurities: Dirt or dust in the finish; may cause small dents to the surface of the finish.
Craters and voids: Spots where paint on the coated surface has receded, often concentrically, to leave a
spot with no paint. Cratering is caused by incompatible foreign materials either in the paint or substrate.
Fisheyes: Circular voids or separation in the coating. Fisheyes are small, crater-like openings in the finish
after it has been applied. They are usually caused by oil, grease, or silicon on the substrate.
Pinholes: Apinhole is a pore-like penetration that ispresent inpaints andcoatings due to the entrapment
of moisture, air, solvents, or other fluids.
Fumes: Contamination from paint fumes. This generally means that small points from another color can
appear on the finish.
Orange Peel: This defect is a rippling of the cured finishing material and appears rough and uneven, much
like the skin of an orange or the exterior of basketball.
Paint Coverage: Ability of a coating to cover the surface on which it’s applied.
Drips: Trace made by the paint while flowing on the substrate
Blisters: Small bubbles or voids on the surface of a molded part caused by trapped gases in the part that
could not escape before the surface began to “skin “during the molding process.COATING AND PLASTICS SPECIFICATION # 01
AESTHETIC
Revision
JUN 21
2022
Page 4 / 5
Burn marks: Black or rust discoloration on an edge or surface, caused by high temperature gases.
Gate marks: Indentation or depression that occurs in the same location of every part due the mold
injection point.
Splay marks: A “splash-like” appearance (or spray pattern) on the surface of a molded part. Often due to
moisture in raw material.
Jetting: Jetting refersto asituationwheremoltenplasticfailsto sticktothemoldsurface dueto the speed
of injection.
Sink Marks: Areas in a molded part where the surface is deformed into a depression. The depressions
typically occur in areas of thick geometry and are caused by uneven cooling.
Weld lines: Areas of a molded part where the molten material has converged after splitting off into two
or more directions in a mold. The hair-like weld line is the result of weak material bonding, which lowers
the strength of the part.
E. INSPECTION STENCIL
150 mm
100 mm
50 mm
0.5mm 0.75mm 1mm 1.5mm 2mm 5mmCOATING AND PLASTICS SPECIFICATION # 01
AESTHETIC
Revision
JUN 21
2022
Page 5 / 5
F. REVISION HISTORY
Revision
Date
Changes / Notes / Comments
Signed by
2022-06-21 Rev 01, header and section F were added. David Maltais
Identifikace uložené verze

SHA-256: 5885779c849da2c287d2b0b2320a5dfd522168e92ef11f6b20051b206aa1910a