https://drive.google.com/file/d/1zttP8qj0ySU1Iz78N5CzVYKqHmW7Q-_g/view ↗ P L A ST I C I N J E C T I O N P R O C E D U R E # 01
Revision FEB 28 2022
MATERIAL REGRIND PROCEDURE Page 1/3
A. OBJECTIVE(S)
Define in a documented manner the method to manage plastic regrind in order to optimize costs while
maintaining part performance, material integrity and reduce demand on natural resources without
compromising quality level of parts produced at TAIGA’s supplier.
B. SCOPE
This procedure covers thermoplastic materials used in polymer processing techniques such as injection
molding, compression molding or extrusion. Only regrind material is in scope, contrary to reprocessed
and recycled material.
C. DEFINITIONS
Hydrolysis: Chemical reaction in which a chemical compound decomposes by reaction with water.
Regrind: Scrap made in-house from the same product being manufactured - runners, parts that are the
wrong color, improperly filled (“short shots”), dimensions that didn’t meet specs, etc.
Reprocessed: Material that is the same manufacturer and grade of material that may have come from
elsewhere, obsolete product, parts of another item that were rejected for the same reasons we would
reject as described as “regrind”.
Recycled: Product made using the same or very similar grades of material, from post consumer scrap, or
end of life products that were not at the end of their useful lives due to age, and most importantly, not
degraded by heat, UV oxidation, chemical attack, contamination, and a whole host of other things that
could have rendered the material “off-spec”.
Thermoplastic: Plastic polymer material that becomes pliable or moldable at a certain elevated
temperature and solidifies upon cooling.
D. PROCEDURE
D.1 GRINDING
The use of reclaimed sprues, runners, and noncontaminated parts is permissible. Use a conventional scrap
grinder equipped with 0.25 in. to 0.375 in. (6.4–9.6mm) screen or similar. Regrind equipment shall be
dedicated to the material used, or an acceptable cleaning method shall be proposed and validated by
TAIGA representative
Under no circumstances parts discarded due to degradation, discoloration or contamination should be
fed to the grinder system. Material that has been degraded because of high moisture content and/or too
long hold-up time in the barrel cannot be re-used.
P L A ST I C I N J E C T I O N P R O C E D U R E # 01
Revision FEB 28 2022
MATERIAL REGRIND PROCEDURE Page 2/3
D.2 STORAGE
Reground resin shall be stringently protected to keep it free of contamination. Whenever possible, the
regrind material should be sent to the dryer as it is generated. When this is not possible, the scrap should
be collected in a closed system and recycled with the same precautions taken for virgin resin.
D.3 DRYING
The regrind shall be blended with virgin material before being added to the dryer. Regrind may require
longer drying times as the reground compound will tend to absorb more moisture than virgin pellets due
to the larger surface area of the regrind. The temperature and drying time shall meet the guideline
provided by the resin manufacturer.
Special attention should be brought to Nylon, Polycarbonate, Polybutadiene terephthalate (PBT) and
Polyethylene terephthalate) (PET) they will undergo hydrolysis in the barrel of the molding machine and
be degraded if not dried properly.
D.4 PROCESSING
Processors may find themselves raising the melt temperature because they have run out of speed due to
a pressure-limited process. Under no circumstances the barrel temperature should be increased above
the resin manufacturer’s recommended limit as this would accelerate polymer degradation and have
negative effect on mechanical properties.
Material processed should have no more than 20% wt. of regrind. The feeding system must demonstrate
its precision and have its calibration up to date. Part by part regrind % must be validated, approved and
documented in the control plan.
In the case of glass fiber reinforced grades, increased loss of strength must be expected due to the
reduction of fiber length which occurs during regrinding. For this reason, no more than 15% wt. of regrind
should be added to reinforced materials.
The regrind feeding strategy (batch/continuous, number of passes, feeding technique, etc.) must be
presented to TAIGA prior to its approval. Regrind shall not affect part performance, fit, function,
appearance.
E. PROCESS CONTROL
E.1 HUMIDITY
The maximum moisture content should be below the value specified by the resin manufacturer in the
technical data sheet (TDS). Value can be measured by a moisture analyzer part of the dryer or by using
portative analyzer.
P L A ST I C I N J E C T I O N P R O C E D U R E # 01
Revision FEB 28 2022
MATERIAL REGRIND PROCEDURE Page 3/3
E.2 MELT FLOW RATE (MFR)
As the resin is reprocessed, its viscosity will tend to decrease and this will result in an increase of the melt
flow rate.
The melt flow rate difference between the feed material and the reference value specified on the TDS
should be of less than 30% using ASTM D1238 method.
E.3 COLOR CHANGE
The color of all the parts produced shall meet the requirements of the following procedure: COATING
AND PLASTICS AESTHETIC SPECIFICATION REV 01.
E.4 TRACKING AND DOCUMENTATION
Control must be put in place to ensure proper tacking and documenting of the actual level of regrind in
every TAIGA parts.
F. REVISION HISTORY
Revision Signed by
Changes / Notes / Comments
Date
2022-06-21 Rev 01, header and section F were added. David Maltais
[READING ORDER TEXT]
PLASTIC INJECTION PROCEDURE # 01
MATERIAL REGRIND PROCEDURE
Revision FEB 28 2022
Page 1 / 3
A. OBJECTIVE(S)
Define in a documented manner the method to manage plastic regrind in order to optimize costs while
maintaining part performance, material integrity and reduce demand on natural resources without
compromising quality level of parts produced at TAIGA’s supplier.
B. SCOPE
This procedure covers thermoplastic materials used in polymer processing techniques such as injection
molding, compression molding or extrusion. Only regrind material is in scope, contrary to reprocessed
and recycled material.
C. DEFINITIONS
Hydrolysis: Chemical reaction in which a chemical compound decomposes by reaction with water.
Regrind: Scrap made in-house from the same product being manufactured - runners, parts that are the
wrong color, improperly filled (“short shots”), dimensions that didn’t meet specs, etc.
Reprocessed: Material that is the same manufacturer and grade of material that may have come from
elsewhere, obsolete product, parts of another item that were rejected for the same reasons we would
reject as described as “regrind”.
Recycled: Product made using the same or very similar grades of material, from post consumer scrap, or
end of life products that were not at the end of their useful lives due to age, and most importantly, not
degraded by heat, UV oxidation, chemical attack, contamination, and a whole host of other things that
could have rendered the material “off-spec”.
Thermoplastic: Plastic polymer material that becomes pliable or moldable at a certain elevated
temperature and solidifies upon cooling.
D. PROCEDURE
D.1 GRINDING
Theuseofreclaimedsprues,runners,andnoncontaminatedpartsispermissible.Useaconventionalscrap
grinder equipped with 0.25 in. to 0.375 in. (6.4–9.6mm) screen or similar. Regrind equipment shall be
dedicated to the material used, or an acceptable cleaning method shall be proposed and validated by
TAIGA representative
Under no circumstances parts discarded due to degradation, discoloration or contamination should be
fed to the grinder system.Material that has been degraded because of high moisture content and/or too
long hold-up time in the barrel cannot be re-used.PLASTIC INJECTION PROCEDURE # 01
MATERIAL REGRIND PROCEDURE
Revision FEB 28 2022
Page 2 / 3
D.2 STORAGE
Reground resin shall be stringently protected to keep it free of contamination. Whenever possible, the
regrind material should be sent to the dryer as it is generated. When this is not possible, the scrap should
be collected in a closed system and recycled with the same precautions taken for virgin resin.
D.3 DRYING
The regrind shall be blended with virgin material before being added to the dryer. Regrind may require
longer drying times as the reground compound will tend to absorb more moisture than virgin pellets due
to the larger surface area of the regrind. The temperature and drying time shall meet the guideline
provided by the resin manufacturer.
Special attention should be brought to Nylon, Polycarbonate, Polybutadiene terephthalate (PBT) and
Polyethylene terephthalate) (PET) they will undergo hydrolysis in the barrel of the molding machine and
be degraded if not dried properly.
D.4 PROCESSING
Processors may find themselves raising the melt temperature because they have run out of speed due to
a pressure-limited process. Under no circumstances the barrel temperature should be increased above
the resin manufacturer’s recommended limit as this would accelerate polymer degradation and have
negative effect on mechanical properties.
Material processed should have no more than 20% wt. of regrind. The feeding system must demonstrate
its precision and have its calibration up to date. Part by part regrind % must be validated, approved and
documented in the control plan.
In the case of glass fiber reinforced grades, increased loss of strength must be expected due to the
reductionoffiber length which occursduring regrinding. For thisreason, no more than 15% wt. of regrind
should be added to reinforced materials.
The regrind feeding strategy (batch/continuous, number of passes, feeding technique, etc.) must be
presented to TAIGA prior to its approval. Regrind shall not affect part performance, fit, function,
appearance.
E. PROCESS CONTROL
E.1 HUMIDITY
The maximum moisture content should be below the value specified by the resin manufacturer in the
technical data sheet (TDS). Value can be measured by a moisture analyzer part of the dryer or by using
portative analyzer.PLASTIC INJECTION PROCEDURE # 01
MATERIAL REGRIND PROCEDURE
Revision FEB 28 2022
Page 3 / 3
E.2MELT FLOW RATE (MFR)
As the resin is reprocessed, its viscosity will tend to decrease and this will result in an increase of the melt
flow rate.
The melt flow rate difference between the feed material and the reference value specified on the TDS
should be of less than 30% using ASTM D1238 method.
E.3COLOR CHANGE
The color of all the parts produced shall meet the requirements of the following procedure: COATING
AND PLASTICS AESTHETIC SPECIFICATION REV 01.
E.4TRACKING AND DOCUMENTATION
Control must be put in place to ensure proper tacking and documenting of the actual level of regrind in
every TAIGA parts.
F. REVISION HISTORY
Revision
Date
Changes / Notes / Comments
Signed by
2022-06-21 Rev 01, header and section F were added. David MaltaisIdentifikace uložené verze